The Gem and Jewelry World's foremost Resource on The Internet.
Re: [Orchid] Casting copper recommendations?  
  [Thread Prev] [Message Prev]      [Date Index]   [Thread Index]      [Message Next] [Thread Next]
From: Terry Ogden
Date: Fri Feb 02 03:12:10 2007
 
     
========[ Invite a Friend - http://www.ganoksin.com/invite.htm  ]========

Noel

>     Does this mean that 90/10 cu/ag will make a good copper solder? 

    In my experiment it did not. 

    I used 26 grains Copper and 2.6 grains Silver, rolled it out to a
    small sheet and cut palions. For soldering it was different. I could
    not get the mix to melt into the joint unless lain on a reflective
    surface when using propane/air. In the third hand, it just would not
    do it with a propane/air torch. Tried butt joining a copper and brass
    strip, used the Oxy/Acet and the brass melted before the
    copper/silver mix. When you do get a joint, it is very strong, even
    stronger than the copper brazing rod, the joint is not as bright
    silver as the rod, but it is lighter than pure copper when it comes
    out of the tumbler. 

    One thing I noticed is that the silver started coming out of the
    copper like it will on Sterling. 

    Positive things are that it pours well, gets really hard, retains
    the copper color, and polishes well. It is a very successful medium
    as described by the poster, but as a solder for copper, I am still
    looking. 

Terry


 
____________________________________________________________________
T h e   O r c h i d   L i s t
Open Electronic Forum for Jewelry Manufacturing Methods and Procedures
____________________________________________________________________
Orchid FAQ:
~ http://www.ganoksin.com/orchid/faq.htm
Orchid Archives:
~ http://www.ganoksin.com/orchid/archive
Orchid Galleries:
~ http://www.ganoksin.com/orchid/gallery.htm
Invite a Friend:
~ http://www.ganoksin.com/invite.htm
____________________________________________________________________
Tips From The Jeweler's Bench - Article Archive
~ http://www.ganoksin.com/borisat/tip_sear.htm
The Jeweler's Selected Bibliography List
~ http://www.ganoksin.com/jewelry-books
Buy Orchid Jewelry:
~ http://www.ganoksin.com/shop
____________________________________________________________________
-Unsubscribe:
-Email: orchid-request AT ganoksin.com Body=unsubscribe subject=blank
____________________________________________________________________

  Click to Visit  
     
  Navigate:  
   
  Orchid Resources:  
   Join & Post
 Invite a friend to join Orchid
 F.A.Q
 Galleries
 BenchExchange
 Orchid Message Archives [Subject Index] [Date Index]

Ganoksin now offers a number of ways for you to stay on top of the latest from Orchid!

  1. My Yahoo - Do you have a My Yahoo page? If so, you can easily read the latest Orchid posts on your personalized page by adding this feed:Add Orchid to My Yahoo!
  2. Add Orchid to myGoogle Add to my Google
  3. Read Orchid with NewsGator and Microsoft Outlook Add Orchid to Your  NewsGator
Support Orchid! - If you believe in what we're doing, you can help!

 
     
     

© Copyright 1996 - 2008, The Ganoksin Project