>     Only when there is a current flowing does the orange peel show. Is
>     it the electricity? 

    I'd double check the polarity. If the current is flowing from the
    piece it will tend to strip it as it is acting like an anode. My
    oldest gold anodes look like this. Positive for the anode, negative
    for the work. Don't rely just on lead wire color. Check your physical
    connections. You didn't mention acid dip and distilled water rinse.
    This step is critical. Also, if the electrocleaner was ever
    overheated its useless. 

    as a test..keeping your setup just as it was use a copper wire on
    your palladium and see what happens. if its correct the copper should
    plate white. 

    Also beware of voltage. Too high a voltage will often frost the
    surface being plated, or too long immersion. Also check that you are
    using the correct anode. 

Good luck
____________________________________________________________________
T h e   O r c h i d   L i s t
Open Electronic Forum for Jewelry Manufacturing Methods and Procedures
____________________________________________________________________
Orchid FAQ:
~ http://www.ganoksin.com/orchid/faq.htm
Orchid Archives:
~ http://www.ganoksin.com/orchid/archive
Orchid Galleries:
~ http://www.ganoksin.com/orchid/gallery.htm
Invite a Friend:
~ http://www.ganoksin.com/invite.htm
____________________________________________________________________
Tips From The Jeweler's Bench - Article Archive
~ http://www.ganoksin.com/borisat/tip_sear.htm
The Jeweler's Selected Bibliography List
~ http://www.ganoksin.com/jewelry-books
Buy Orchid Jewelry:
~ http://www.ganoksin.com/shop
____________________________________________________________________
-Unsubscribe:
-Email: orchid-request AT ganoksin.com Body=unsubscribe subject=blank
____________________________________________________________________

  Click to Visit  
     
  Navigate:  
   
  Orchid Resources:  
   Join & Post
 Invite a friend to join Orchid
 F.A.Q
 Galleries
 BenchExchange
 Orchid Message Archives [Subject Index] [Date Index]

Ganoksin now offers a number of ways for you to stay on top of the latest from Orchid!

  1. My Yahoo - Do you have a My Yahoo page? If so, you can easily read the latest Orchid posts on your personalized page by adding this feed:Add Orchid to My Yahoo!
  2. Add Orchid to myGoogle Add to my Google
  3. Read Orchid with NewsGator and Microsoft Outlook Add Orchid to Your  NewsGator
Support Orchid! - If you believe in what we're doing, you can help!

 
     
     

© Copyright 1996 - 2008, The Ganoksin Project