>     Argentium Experimentation (casting) I had a conversation with one
>     of my casters in RI today about their recent experience with
>     Argentium. The upside is that it casts with no noticeable pitting-
>     very dense castings. They were able to cast it successfully on
>     their first attempt using a casting machine with an inert gas
>     atmosphere. They were casting handles for a client's project. A
>     boon for silversmiths. The downside, at least for the present, is
>     its cost- about $4 per ounce more than sterling. I was told that it
>     cannot be re-melted for additional casting, and that about 60% is
>     used up by sprue trees in a (for them) typical 15 ounce cast.
>     Roughly, it is about 3 times as expensive to cast in Argentium, 

Hi Rick,

    I don't do my own casting, but my understanding is that Argentium
    Sterling Silver CAN be re-used for casting, but one must be careful
    to have at least 50% of the casting be fresh, new silver, (and no
    more than 50% be re-used silver). I suggest that you casters talk to
    the folks at info AT argentiumsilver.com, who will put your caster in
    touch with folks experienced at casting Argentium Sterling, and
    verify my info. 

Cindy
Cynthia Eid
http://www.cynthiaeid.com

____________________________________________________________________
T h e   O r c h i d   L i s t
Open Electronic Forum for Jewelry Manufacturing Methods and Procedures
____________________________________________________________________
Orchid FAQ:
~ http://www.ganoksin.com/orchid/faq.htm
Orchid Archives:
~ http://www.ganoksin.com/orchid/archive
Orchid Galleries:
~ http://www.ganoksin.com/orchid/gallery.htm
Invite a Friend:
~ http://www.ganoksin.com/invite.htm
____________________________________________________________________
Tips From The Jeweler's Bench - Article Archive
~ http://www.ganoksin.com/borisat/tip_sear.htm
The Jeweler's Selected Bibliography List
~ http://www.ganoksin.com/jewelry-books
Buy Orchid Jewelry:
~ http://www.ganoksin.com/shop
____________________________________________________________________
-Unsubscribe:
-Email: orchid-request AT ganoksin.com Body=unsubscribe subject=blank
____________________________________________________________________

  Click to Visit  
     
  Navigate:  
   
  Orchid Resources:  
   Join & Post
 Invite a friend to join Orchid
 F.A.Q
 Galleries
 BenchExchange
 Orchid Message Archives [Subject Index] [Date Index]

Ganoksin now offers a number of ways for you to stay on top of the latest from Orchid!

  1. My Yahoo - Do you have a My Yahoo page? If so, you can easily read the latest Orchid posts on your personalized page by adding this feed:Add Orchid to My Yahoo!
  2. Add Orchid to myGoogle Add to my Google
  3. Read Orchid with NewsGator and Microsoft Outlook Add Orchid to Your  NewsGator
Support Orchid! - If you believe in what we're doing, you can help!

 
     
     

© Copyright 1996 - 2008, The Ganoksin Project