Hello All -

    I worked for a small jewelry manufacturer many years ago and spent
    some time troubleshooting our investment/casting issues.  

    We daringly tried an experiment on some injection waxes that
    produced amazingly cleaner castings. 

    After the wax models/sprues are added to the rubber base try
    spraying the whole thing with a spray bottle mixture of room temp.
    water and about 1/2 teaspoon of mild dishwashing liquid.  Let it
    stand on the waxes for about a minute and then rinse off under
    gently running tepid water.  Use an air-gun (low pressure) to blow
    the excess water off and dry the tree... then invest as usual. Yes,
    you'll need an airline in your studio. 

    This step will remove hand oils, lint, small particles of wax dust
    and any other surface dirt that may be stuck on the waxes and
    sprues.  

    If you already do this process, good for you !  It does make a
    difference. 

    Thanks to some great people that I worked with, this step gave us
    better surface quality on our castings ! 

Ciao,
Margie Mersky "The Wax Maven"
www.mmwaxmodels.com

____________________________________________________________________
T h e   O r c h i d   L i s t
Open Electronic Forum for Jewelry Manufacturing Methods and Procedures
____________________________________________________________________
Orchid FAQ:
~ http://www.ganoksin.com/orchid/faq.htm
Orchid Archives:
~ http://www.ganoksin.com/orchid/archive
Orchid Galleries:
~ http://www.ganoksin.com/orchid/gallery.htm
Invite a Friend:
~ http://www.ganoksin.com/invite.htm
____________________________________________________________________
Tips From The Jeweler's Bench - Article Archive
~ http://www.ganoksin.com/borisat/tip_sear.htm
The Jeweler's Selected Bibliography List
~ http://www.ganoksin.com/jewelry-books
Buy Orchid Jewelry:
~ http://www.ganoksin.com/shop
____________________________________________________________________
-Unsubscribe:
-Email: orchid-request AT ganoksin.com Body=unsubscribe subject=blank
____________________________________________________________________

  Click to Visit  
     
  Navigate:  
   
  Orchid Resources:  
   Join & Post
 Invite a friend to join Orchid
 F.A.Q
 Galleries
 BenchExchange
 Orchid Message Archives [Subject Index] [Date Index]

Ganoksin now offers a number of ways for you to stay on top of the latest from Orchid!

  1. My Yahoo - Do you have a My Yahoo page? If so, you can easily read the latest Orchid posts on your personalized page by adding this feed:Add Orchid to My Yahoo!
  2. Add Orchid to myGoogle Add to my Google
  3. Read Orchid with NewsGator and Microsoft Outlook Add Orchid to Your  NewsGator
Support Orchid! - If you believe in what we're doing, you can help!

 
     
     

© Copyright 1996 - 2008, The Ganoksin Project