    Hi Donna.  I have not done depletion guilding on 22K gold, but have
    done copper depletion on sterling in order to bring up the fine
    silver to the surface. When doing this process on silver, I heat the
    silver gently until it discolors, then  put it in the sparex pickle,
    until the silver is free of discoloration. I do this as many times as
    necessary---which will be determined by the fact that when heating
    with the torch, the silver no longer turns black. With gold, there
    may be two problems you are contending with. One is that  part of the
    alloy in the gold has zinc, or another metal which is incompatible
    with enameling. If the alloy is not the problem, it may be that you
    are not heating, picking, heating and pickling a sufficient number of
    times to rid the gold of the copper and thereby you are not bringing
    the pure gold to the surface. Perhaps some of the other enamelists
    may  have some other suggestions.  It might be a good idea to
    contact Tom Ellis or Bill Helwig at Thompson enamel for their advice 

  Alma

____________________________________________________________________
T h e   O r c h i d   L i s t
Open Electronic Forum for Jewelry Manufacturing Methods and Procedures
____________________________________________________________________
Orchid FAQ:
~ http://www.ganoksin.com/orchid/faq.htm
Orchid Archives:
~ http://www.ganoksin.com/orchid/archive
Orchid Galleries:
~ http://www.ganoksin.com/orchid/gallery.htm
Invite a Friend:
~ http://www.ganoksin.com/invite.htm
____________________________________________________________________
Tips From The Jeweler's Bench - Article Archive
~ http://www.ganoksin.com/borisat/tip_sear.htm
The Jeweler's Selected Bibliography List
~ http://www.ganoksin.com/jewelry-books
Buy Orchid Jewelry:
~ http://www.ganoksin.com/shop
____________________________________________________________________
-Unsubscribe:
-Email: orchid-request AT ganoksin.com Body=unsubscribe subject=blank
____________________________________________________________________

  Click to Visit  
     
  Navigate:  
   
  Orchid Resources:  
   Join & Post
 Invite a friend to join Orchid
 F.A.Q
 Galleries
 BenchExchange
 Orchid Message Archives [Subject Index] [Date Index]

Ganoksin now offers a number of ways for you to stay on top of the latest from Orchid!

  1. My Yahoo - Do you have a My Yahoo page? If so, you can easily read the latest Orchid posts on your personalized page by adding this feed:Add Orchid to My Yahoo!
  2. Add Orchid to myGoogle Add to my Google
  3. Read Orchid with NewsGator and Microsoft Outlook Add Orchid to Your  NewsGator
Support Orchid! - If you believe in what we're doing, you can help!

 
     
     

© Copyright 1996 - 2008, The Ganoksin Project