    I wonder why nobody else referred to this method, - therefore this
    post: Use the following: 

    Potassium nitrate  KNO2  4 parts per weight 

    Potassiumaluminumsulphate  KAl(SO4)2, 12 H2O 2 ppw and 

    Sodium chloride (salt)  2 ppw 

    Add water till a thin slurry is reached. Fill into a fireproof
    container (not metallic) and boil. 

    Suspend the item to be 'surface enriched' from a silver wire into
    the solution and let boil for 10 - 20 minutes. Clean and scratch
    brush. Repeat as necessary. 

    A warning: Do not let the piece rest on the bottom, it simply
    dissolves (I speak from experience :-) 

    I think I owe this recipe from a previous posting here on Orchid,
    but could not find it in the archives. However, it has worked for me. 

    Regards from Niels on Bornholm, Denmark, where snow has poured down
    all day and extinguished our hopes for spring (at least for a few 
days) 


____________________________________________________________________
T h e   O r c h i d   L i s t
Open Electronic Forum for Jewelry Manufacturing Methods and Procedures
____________________________________________________________________
Orchid FAQ:
~ http://www.ganoksin.com/orchid/faq.htm
Orchid Archives:
~ http://www.ganoksin.com/orchid/archive
Orchid Galleries:
~ http://www.ganoksin.com/orchid/gallery.htm
Invite a Friend:
~ http://www.ganoksin.com/invite.htm
____________________________________________________________________
Tips From The Jeweler's Bench - Article Archive
~ http://www.ganoksin.com/borisat/tip_sear.htm
The Jeweler's Selected Bibliography List
~ http://www.ganoksin.com/jewelry-books
Buy Orchid Jewelry:
~ http://www.ganoksin.com/shop
____________________________________________________________________
-Unsubscribe:
-Email: orchid-request AT ganoksin.com Body=unsubscribe subject=blank
____________________________________________________________________


  Click to Visit  
     
  Navigate:  
   
  Orchid Resources:  
   Join & Post
 Invite a friend to join Orchid
 F.A.Q
 Galleries
 BenchExchange
 Orchid Message Archives [Subject Index] [Date Index]

Ganoksin now offers a number of ways for you to stay on top of the latest from Orchid!

  1. My Yahoo - Do you have a My Yahoo page? If so, you can easily read the latest Orchid posts on your personalized page by adding this feed:Add Orchid to My Yahoo!
  2. Add Orchid to myGoogle Add to my Google
  3. Read Orchid with NewsGator and Microsoft Outlook Add Orchid to Your  NewsGator
Support Orchid! - If you believe in what we're doing, you can help!

 
     
     

© Copyright 1996 - 2007, The Ganoksin Project