>      Hello people, A little help please. I'm trying to get 24Kt foil
>     over the japanese alloy Shibuishi with little luck. <snip>

    Mac, The problem seems to me to be one of metallurgy. The gold foil
    should be bonded to fine silver and the high copper content of
    shibuichi may be the source of your problems. If you want to bond the
    gold by using a diffusion bonding process, you are going to need a
    fine silver surface to attach the foil to. I can think of a couple of
    possible ways of doing this: 

    1. Use depletion gilding to bring up an area of fine silver. This
    involves heating, pickling, and brass brushing repeatedly for 4 or 5
    cycles. It may be a challenge to find a way to perform the process
    on only one area of the piece. 

    2. Bond a piece of fine silver to the shibuichi first using a
    process similar to silver granulation. Once the fine silver is in
    place, bond the fine gold to the silver surface. You would need to
    have both the silver and gold foils cut to the exact same shape and
    have good alignment. 

    3. Similar to number 2, but make some bi-metalic foil of fine silver
    and fine gold bonded together. Then attach the bi-metal foil, gold
    side up, to the shibuichi. I think this is the best approach.
    Although it may take some work to make the bi-metal and roll it out,
    it would be a one step process to attach it in it's final form. 

    Just a few quick ideas. With a bit of experimentation, you should be
    able to get it to work. Email me off list if I can be of further
    assistance. 

Good Luck,
Jim DeRosa
James DeRosa, Jr.
140 Clifton Drive
Boardman, OH  44512-1616
330-782-0702

____________________________________________________________________
T h e   O r c h i d   L i s t
Open Electronic Forum for Jewelry Manufacturing Methods and Procedures
____________________________________________________________________
Orchid FAQ:
~ http://www.ganoksin.com/orchid/faq.htm
Orchid Archives:
~ http://www.ganoksin.com/orchid/archive
Orchid Galleries:
~ http://www.ganoksin.com/orchid/gallery.htm
Invite a Friend:
~ http://www.ganoksin.com/invite.htm
____________________________________________________________________
Tips From The Jeweler's Bench - Article Archive
~ http://www.ganoksin.com/borisat/tip_sear.htm
The Jeweler's Selected Bibliography List
~ http://www.ganoksin.com/jewelry-books
Buy Orchid Jewelry:
~ http://www.ganoksin.com/shop
____________________________________________________________________
-Unsubscribe:
-Email: orchid-request AT ganoksin.com Body=unsubscribe subject=blank
____________________________________________________________________


  Click to Visit  
     
  Navigate:  
   
  Orchid Resources:  
   Join & Post
 Invite a friend to join Orchid
 F.A.Q
 Galleries
 BenchExchange
 Orchid Message Archives [Subject Index] [Date Index]

Ganoksin now offers a number of ways for you to stay on top of the latest from Orchid!

  1. My Yahoo - Do you have a My Yahoo page? If so, you can easily read the latest Orchid posts on your personalized page by adding this feed:Add Orchid to My Yahoo!
  2. Add Orchid to myGoogle Add to my Google
  3. Read Orchid with NewsGator and Microsoft Outlook Add Orchid to Your  NewsGator
Support Orchid! - If you believe in what we're doing, you can help!

 
     
     

© Copyright 1996 - 2008, The Ganoksin Project